Aluminium comparison table
Wrought aluminium alloys
Naturally hardenable |
1000-series |
3000-series |
4000-series |
5000-series |
8000-series |
Alloys are harden with alloying and cold working |
Work-hardenable |
2000-series |
6000-series |
7000-series |
|
|
Alloys are harden with precipitation hardening |
Common aluminium alloys; analysis and properties
AW |
|
Si |
Fe |
Cu |
Mn |
Mg |
Cr |
Zn |
Ti |
Temper |
Rp0,2 min |
Rm min |
Rm max |
A50 mm % |
T-radius 90° |
1050A |
Al 99.5 |
0.25 |
0.4 |
0.05 |
0.05 |
0.05 |
-- |
0.07 |
0.05 |
H22 |
55 |
85 |
125 |
5 |
0 t |
2017A |
AlCu4MgSi |
0.20-0.8 |
0.7 |
3.5-4.5 |
0.40-1.0 |
0.40-1.0 |
0.1 |
0.25 |
-- |
T4 |
245 |
390 |
-- |
14 |
3.0 t |
2024 |
AlCu4Mg1 |
0.5 |
0.5 |
3.8-4.9 |
0.3-0.9 |
1.2-1.8 |
0.1 |
0.25 |
0.15 |
T4 |
290 |
425 |
-- |
12 |
4.0 t |
3103 |
AlMn1 |
0.5 |
0.7 |
0.1 |
0.9-1.5 |
0.3 |
0.1 |
0.2 |
-- |
H22 |
75 |
115 |
155 |
7 |
0.5 t |
4017 |
AlSiMnMgCu |
0.6-1.6 |
0.7 |
0.10-0.50 |
0.6-1.2 |
0.10-0.50 |
-- |
0.2 |
-- |
|
|
|
|
|
|
5005 |
AlMg1 |
0.3 |
0.7 |
0.2 |
0.2 |
0.5-1.1 |
0.1 |
0.25 |
-- |
H22/H32 |
80 |
125 |
165 |
5 |
0.5 t |
5026 |
AlMg4.5MnSiFe |
0.55-1.4 |
0.20-1.0 |
0.10-0.30 |
0.6-1.8 |
3.9-4.9 |
0.3 |
1 |
0,2 |
H24 1) |
220 |
300 |
340 |
5 |
-- |
5083 |
AlMg4.5Mn0.7 |
0.4 |
0.4 |
0.1 |
0.40-1.0 |
4.0-4.9 |
0.05-0.25 |
0.25 |
0.15 |
H22/H32 |
215 |
305 |
380 |
6 |
1.5 t |
5754 |
AlMg3 |
0.4 |
0.4 |
0.1 |
0.5 |
2.6-3.6 |
0.3 |
0.15 |
0.15 |
H22/H32 |
130 |
220 |
270 |
8 |
1.0 t |
6063 |
AlMg0.7Si |
0.2-0.6 |
0.35 |
0.1 |
0.1 |
0.45-0.9 |
0.1 |
0.1 |
0.1 |
T4 |
65 |
130 |
-- |
12 |
-- |
6082 |
AlSi1MgMn |
0.7-1.3 |
0.5 |
0.1 |
0.40-1.0 |
0.6-1.2 |
0.25 |
0.2 |
0.1 |
T4 |
110 |
205 |
-- |
12 |
1.5 t |
7075 |
AlZn5.5MgCu |
0.4 |
0.5 |
1.2-2.0 |
0.3 |
2.1-2.9 |
0.18-0.28 |
5.1-6.1 |
0.2 |
T6 |
460 |
540 |
-- |
6 |
5.5 t |
Yield- ja tensile strengths as MPa. Material thickness 1mm
(1) Thickness 3-12,5 mm
Common EN-standards for aluminiums
EN 485-2 |
Aluminium and aluminium alloys. Sheet,strip and plate. Part 2: Mechanical properties |
EN 485-3 |
Aluminium and aluminium alloys. Sheet,strip and plate. Part 3: Tolerances on dimensions and form for hot-rolled products |
EN 485-4 |
Aluminium and aluminium alloys. Sheet,strip and plate. Part 3: Tolerances on shape and dimensions for cold-rolled products |
EN 515 |
Aluminium and aluminium alloys - Wrought products - Temper designations |
EN 573-1 |
Aluminium and aluminium alloys. Chemical composition and form of wrought products. Part 1: Numerical designation system |
EN 573-2 |
Aluminium and aluminium alloys. Chemical composition and form of wrought products. Part 2: Chemical symbol based designation system |
EN 573-3 |
Aluminium and aluminium alloys. Chemical composition and form of wrought products. Part 3: Chemical composition and form of products |